How to cut > How to avoid softening with thermal cutting

How to reduce the risk of softening

The best way of eliminating the risk of softening is to use cold cutting methods, such as abrasive water jet cutting. If thermal cutting must be performed, laser or plasma cutting is preferable to oxy-fuel cutting, as oxy-fuel cutting subjects the workpiece to higher levels of heat compared to plasma or laser cutting.

For oxy-fuel cutting, an effective way of limiting and reducing the extent of the soft zone is to water-cool the plate and the cut surface during the cutting operation. This can be achieved either by submerging the plate in water or by spraying water on the piece during and after cutting. However, even with submersion or water spraying, a soft zone will still develop in the cutting edge within approximately 5-10 mm (0.197 – 0.394”). This occurs because any water is pushed away by the ignition flame and the cutting oxygen jet preventing the water from cooling the cutting front until after softening has occurred. Nevertheless, water cooling can prevent "global" softening of the component. 

Submerged cutting can be done with both plasma cutting and oxy-fuel cutting, offering several advantages such as:

  • Prevents loss of hardness of the entire component
  • Reduced distortion of the cut piece
  • Pieces are cooled directly after cutting 
  • No fumes or dust
  • Reduced noise level

Submerged cutting

Since preheating is not applicable for submerged cutting, the only available measures to counteract the risk for hydrogen cracking are postheating and reduced cutting speed. When small pieces are cut from thick Hardox® wear plate using oxy-fuel, there is risk of softening and cut edge cracking. This is best avoided through submerged cutting at low cutting speeds or by post-heat treatment of the cut pieces, which can be done with a torch or in a furnace.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein.