Strenx performance steel

Strenx® 110 XF

Download data sheet

Dimension Range

Strenx® 110 XF is available in thicknesses of 2.0 - 10.0 mm, and in widths up to 1600 mm as coil, slit coil and cut to length sheets in lengths up to 16000 mm.

Mechanical Properties

Thickness
(mmin)
Thickness
(mmin)
2.00 - 10.000.079 - 0.393
Yield strength ReH 1)
(min MPaksi)
760110
Tensile strength Rm
(min MPaksi)
813118
Elongation A50
(min %)
12

The mechanical properties are tested in the transverse direction.

Testing can also be performed in the longitudinal direction, according to requirements in EN 10149-2 S700MC and ASTM A1011 grade 100 on request.

1) If ReH is not applicable then Rp0.2 is used.

Impact Properties

Product
Product
Strenx® 110 XF
Min. impact energy for longitudinal testing,
Charpy V 10x10 mm test specimen
27 J / -40 °C20 ft-lbs / -40 °F

Impact testing according to EN ISO 148-1 is performed on thicknesses ≥ 6 mm. The specified minimum value corresponds to a full-size specimen.

Bending Properties

Bending
Bending
Min. inner bending radius for a 90° bend
t < 3.00 mm
0.8 xt
3.00 ≤ t ≤ 6.00 mm
1.2 xt
t > 6.00 mm
1.6 xt

Valid in both the longitudinal and transverse direction.

Chemical Composition (ladle analysis)

C
(max %)
C
(max %)
0.12
Si
(max %)
0.03
Mn
(max %)
2.10
P
(max %)
0.020
S
(max %)
0.010
Al
(min %)
0.015
Nb
(max %)
0.09 1)
V
(max %)
0.20 1)
Ti
(max %)
0.15 1)

Strenx® 110 XF is available with different levels of Si: from max 0.03%, up to max 0.28%. Max Si 0.03% is the standard version that is suitable for hot dip galvanizing with thin Zinc layers, and for products that will not be galvanized. If the material is to be hot-dip galvanized and a thicker Zinc layer is requested, this must be specified at the time of order.

1) Sum of Nb, V and Ti = max 0.22%.

Tolerances

More details are given in SSAB’s brochure Strenx® Guarantees.

Thickness

Tolerances according to Strenx® Thickness Guarantees.

Strenx® Guarantees offer considerably narrower thickness tolerances compared to EN 10051. 

Length and Width

Width and length tolerances according to SSAB standard.

The SSAB standard offer narrower width and length tolerances compared to EN 10051.

Length tolerances only apply for cut to length sheets.

Shape

Tolerances according to EN 10051.

Narrower tolerances according to the SSAB standard are available on request 

Flatness

Tolerances according to Strenx® Flatness Guarantees Class A.

Strenx® Flatness Guarantees offer narrower tolerances compared to EN 10051.

Flatness guarantees only apply for cut to length sheets. 

Surface Properties

According to EN 10163-2 Class A, Subclass 3.

Delivery Conditions

Thermomechanically Rolled. Strenx® 110 XF is available in as rolled or pickled surface condition with mill or cut edge.

Fabrication and Other Recommendations

Welding, bending and machining

Strenx® 110 XF has good welding, cold forming and cutting performance. Strenx® 110 XF is a cold forming steel not suited for heat treatments at temperatures above 1080°F (580°C) since the material then may lose its guaranteed properties.

For information concerning fabrication, see SSAB´s brochures on www.ssab.com or consult Tech Support.

Appropriate health and safety precautions must be taken when bending, welding, cutting, grinding or otherwise working on the product.

Strenx® 110 XF high-strength structural steel

Strenx® 110 XF is a cold forming high-strength structural steel. It is a thermomechanically rolled product with a minimum yield strength of 110 ksi. It is suitable for a wide range of structural applications, including equipment and components in the transport, lifting and agriculture industry. Strenx® 110 XF meets the requirements of EN 10149-2 S700MC, ASTM A1011 grade 100 and ASTM A1018 grade 100 and can be supplied according to all of these standards' specifications on request. Strenx® 110 XF is available in thicknesses of 0.079 - 0.393 inches, and in widths up to 63 inches as coil, slit coil and cut to length sheets in lengths up to 630 inches.

Get technical advice

Show specs in:

MetricImperial