How to cut > How to avoid softening with thermal cutting

Heat affected zone (HAZ) after thermal cutting of QT-steels

Thermal cutting inevitably leads to the formation of a Heat Affected Zone (HAZ) independent of the steel grade. In the case of quenchable steels, the HAZ can be divided into two distinct zones: a re-quenched zone and a tempered zone (see graph below).

Zone 1 and 2

The peak temperature of the material at certain distances from the cut edge is depicted in the graph below.

Peak temperature from the cut edge

The outermost part of the HAZ, situated approximately 1-2 mm (0.039-0.079 inches) from the cut edge, experiences temperatures exceeding 900°C (482°F) during the cutting process. As the cutting torch progresses, heat rapidly disperses into the plate, causing Zone 1 to cool so rapidly that it undergoes re-quenching. 

Consequently, the hardness and strength of this zone are higher than in other parts of the HAZ and the unaffected parent metal. Zone 2, positioned between Zone 1 and the unaffected parent material, is heated to temperatures below 900°C (1,652°F) during cutting. The material in Zone 2 undergoes tempering due to the heat generated during cutting operations. Hardness values in this zone vary depending on the steel grade and the efficiency of the cutting process.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein.